News & Insights

From Coil to Coating: How Hot Dip Galvanized Flat Bar Is Made

2026-11-28 09:40:42 0

Coating thickness is set by the process, not by a promise. Understanding the eight steps explains why two suppliers quoting the same 85 microns can deliver very different service life.

1. Incoming inspection

Check grade, section tolerance and surface. Heavy rust or lamination must be removed or the bar rejected, because no coating can bond to a cracked surface.

2. Pickling

Hydrochloric acid at 10 to 15 percent removes mill scale, typically 20 to 60 minutes at ambient temperature, until the surface is uniformly grey. Over pickling causes pitting and hydrogen uptake, under pickling leaves scale that later lifts the coating.

3. Rinsing and fluxing

Two water rinses then a zinc chloride and ammonium chloride flux bath at 60 to 80 C. The salt film prevents re-oxidation and helps the zinc wet the steel. Flux concentration and iron content are checked daily; this is where most small plants get bubbles and skip coating.

4. Drying

80 to 120 C to remove moisture. Water entering the kettle causes explosions and gas pores in the coating.

5. Galvanizing

445 to 455 C, immersion 1 to 5 minutes. Too hot and the alloy layer grows brittle and grey; too cold and the zinc is sluggish, leaving uncoated patches.

6. Air knife and cooling

High pressure air wipes excess zinc back into the kettle and sets the coating weight. Parts then cool below 200 C so the alloy layer stops growing.

7. Passivation and straightening

A passivation film prevents white rust in transit. Bars are then straightened and cut to 6 m or to drawing.

8. Inspection and packing

Coating checked with a magnetic gauge, appearance checked for skip, lumps and black spots, dimensions and straightness checked. Then bundles on timber, labelled with heat number and coating report.